CHAIRMAKER’S JOURNAL

Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #10: Post Bend Shaping—Rear Legs, Part 1

Evaluating each leg for flatness  |  Joint on side flat  |  Thickness the legs to final dimension  |  Trimming the curved rear legs to length

The bending is complete and the rear legs have been drying in my drying closet for about a week. I always check the moisture content before removing the legs from the forms. In this case the legs have dried to about 8 or 9% moisture content so I remove them from the forms. I’m now ready to begin the post bend shaping. When this is complete the legs will be ready for cutting the slat mortises.

Evaluate each leg for flatness

The bending process almost always introduces some twist in the leg. If you remember from the post on preparing the rear leg blanks for bending, the width front-to-back is 1-5/8″ and the width side-to-side is 1-7/8″. The extra 1/4″ side-to-side is there to allow me to mill out any twist that is introduced during bending. To begin I need to evaluate each leg in order to choose the best side to joint flat. I have found that one side generally pivots in the center of the leg and that the opposite side, although not flat, tends to be more stable with points at each end touching the bench top. This photo shows the side of the leg that pivots in the center. This side is facing down on the bench top and you can see that the center touches the bench top while both ends of the leg rise above it, especially on the right.

The next photo shows the same leg flipped over to the other side. As you can see, that although it is not entirely flat, it is pretty close. This is the side I will joint, mainly because it already much closer to flat and it will be much more stable passing it across the jointer. I don’t normally clamp the leg to the bench top to evaluate it for flatness, but I needed some way to hold it in place so that I could photograph these two examples. Usually I simply press the leg against a flat surface to see which side is best.

Joint one side flat

Now I am ready to flatten the preferred side on the jointer. One of the benefits for my students is that the machinery I have is typical of that found is many amateur shops. My jointer, a 6″ model by Ridgid, is not ideal for jointing a leg of this length since the beds are only 22″ long on either side of the cutter head, so I have had to develop strategies to get a good result. A professional shop might have a 12″ or even a 16″ jointer with a bed long enough to get the entire length of the leg on the table on both sides of the cutter head—jointing using a machine such as this would be much simpler, but students usually don’t have this type of equipment.

This series of illustrations shows the process I use when jointing. The jointer can be a dangerous tool so be sure to use appropriate push blocks that will keep your hands safely away from the cutter head and follow the manufacturer’s safety instructions. I like to start with the bottom half of the leg leading into the cut because this end of the leg is wider and more stable. As I pass the leg over the cutter head I change the position of my hands so that downward and forward pressure is applied across as much of the length of the leg as possible as shown in the steps below. Depending on the initial flatness of the leg it usually take two or three passes to flatten. With a very twisted leg it can take even more. Remember that the leg is 1/4″ oversize so there’s quite a lot of extra material to work with. Once I have flattened one side I label it with a “J” so I know it is the jointed side.

Thickness to final dimension

The next step is to thickness both legs down to the final side-to-side dimension of 1-5/8″. With the jointed side down I pass each leg through the thickness planer. After each pass I turn the wheel a half turn (1/32″) and make another cut. I measure my progress with a combination square set at 1-5/8″ and stop when I reach final thickness.

Trim to final length

This next step may sound simple, but as with most of the processes in the making of this chair, it involves subtleties that are worth paying attention to. The primary issue is that the legs are curved and it’s possible that they may have slightly different bends. A small difference in bend can affect the length of the leg as measured from bottom to top as shown in the illustration below. This in turn can have the effect of one leg appearing taller than the other in the final chair. This is especially important if I am working on a set of chairs and I want a consistent visual appearance from one chair to the next. So I can’t simply trim equal amounts off the top and equal amounts off the bottom of each leg since this will not account for any differences in the bend. 

To deal with this issue there is a method for cutting curved parts to length on the chop saw. I begin by setting a stop at 42-3/16″ relative to the blade set for a 90° cut. Next I place a small block against the fence and the stop. Then I clamp another block to fence so that it’s touching the blade as shown in the photo on the left. These two blocks can vary in length but should be the same thickness. The purpose of these blocks is to keep the cut-off from touching the right side of the fence as shown in the photo on the right. This is extremely important for making a safe cut. If the cut-off contacts the fence during the cut the blade will bind causing kick-back. To reiterate, there MUST be a gap between the end of the leg being cut and the fence on the right side of the blade.

Finally rotate the blade to an open angle of 103°. Here is the saw set up and ready for the first cut.

Place the top of the leg against the stop and hold the bottom of the leg against the block next to the blade. Make the first cut. This will trim about 1-1/4″ off the bottom of the leg.

After trimming the bottom on both legs move the stop 3" closer to the blade. This will put the stop at 39-3/16″ from the blade set at 90°. Keep the blade at an open angle of 103°. Place the bottom of the leg against the stop and hold the top of the leg against the block next to the blade. Make the cut. This will trim about 3-1/8″ off the top of the leg.

Here are both rear legs jointed flat, thicknessed to 1-5/8″, and trimmed to final length.

Those of you who were paying very close attention to the photos of the chop saw set-up may have noticed the old sign in the window behind and to the left of the saw. It very emphatically states in all capital letters “POSITIVELY NO DIPPING FOR MINNOWS ALLOWED. Dr. E. W. MILLER”. We found the sign in one of the outbuildings when we moved here more than 30 years ago. I believe Dr. Miller lived in our house during the 30s and 40s. There is a small creek in front of the house that nowadays has water in it some of the time. Back then it must have flowed all year round. I sometimes try to imagine what prompted Dr. Miller to go to the trouble and expense of putting up this sign. In my mind’s eye I see bands of marauding teenagers causing so much trouble dipping for minnows that it compelled action. Times have changed.

In the next post I’ll use a combination of hand tools and a band saw for the two additional shaping steps required before the legs are ready for slat mortising.

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #9: Bending the Slats

Dimensions for the slat bending form and slat drying form  |  Bend the slats  |  Dry the slats  |  Source of supply for the slat bending strap

Now that I have milled slat blanks it’s time to bend. Normally I mill the slats while the rear legs are in the steam box then steam and bend the slats after I bend the rear legs. If I am steaming the slats in a separate session I wait for temperature in the steam box to reach 200° before putting the slats in the box and counting the time. I put the slats into a small rack and then into the steam box. After 20 minutes they are ready to bend. There are two forms used in the slat bending process: a bending form (front) and a drying form (rear).

A large contributor to a successful bend is doing things in a consistent manner. If you are inconsistent and there are problems, it will be very difficult to figure out the source. A consistent process, on the other hand, allows you to isolate each step to determine the source of a problem. This is a general principle in every aspect of building this chair, but especially in steam bending. First, the moisture content of the slat should be between 12% and 20% (if it is much higher be sure to make the blank a little thicker to allow for shrinkage during drying). Steam time is normally 20 minutes at 200°. The bending form is a half circle with a radius of 9-3/4″. This shape actually over bends the slat in much the same way that the rear legs are over bent. And since the arc of the form is a true half circle every part of the slat will receive the same amount of over bend, and the amount of over bend will be very consistent from one slat to the next resulting is slats with a very consistent arc. Finally, I am very careful to hold each slat in the form for the same amount of time.

The size of this form will accommodate the smallest slats for the side chair up to the largest slats for the rocking chair. The main part of the form is made from 6 layers of 3/4″ plywood laminated together using screws. Here are the dimensions and details. A source for stainless steel is listed below.

The drying form is simply a sheet of 3/4″ plywood with four cleats. Each cleat has a 1/4″ wide angled notch that captures the end of the slat. The distance between the notches is very important. In this case it is 18-1/2″ so that a slat blank that is 20″ in length will have the correct amount of bend when captured between the two cleats. The angle of this bend is actually a little more than what is actually necessary—each slat will be individually flattened to the final angle at a later point in the process.

Steps for steam bending slats:

  • Steam slats for 20 minutes at 200°
  • Remove one slat from the steam box
  • Place the slat in the form and if one side is marked as front place it facing down on the form
  • Push the bending strap down as far as it will go, clamp, and hold for 15 seconds
  • Release the bending strap, remove the slat and rotate it end-for-end
  • Place the slat back in the form, clamp, and hold for another 45 seconds
  • Release the bending strap and remove the slat
  • Press the slat into the drying form
  • Repeat for each slat
  • Place the drying form in a dry place for several days to allow the slats to dry

Here’s a video that shows the entire process. Or watch it directly on YouTube.

Here are the slats in the drying form. I will put the form in my drying closet for several days to dry. If you don’t have a drying closet any warm and dry space will do. Once the slats are dry they sometimes will literally fall out of the form. 

And here is the chair so far. I have rough milled all of the blank parts and final milled and bent the rear legs and slats. In this photo the rear legs are in front, the slats are behind them (with one extra slat), rung blanks are in the back on the left, and front leg blanks are in the back on the right.

In the next post I will begin the post-bend shaping of the rear legs in preparation for cutting the slat mortises.

Source • Stainless Steel: 304 Stainless Steel, 2B Finish, 16 Gauge (.0595″), 4-1/2″ x 30″, Stainless Supply

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #8: Prepare Slats for Steam Bending

Transform a rough, quarter sawn slat blank into individual slat blanks ready for steam bending

If you remember from the post on milling blank parts, I cut the slat blank from clear, quarter sawn stock. It is about 4-1/2″ wide x 22″ long x 9/4 thick. Here is the rough blank.

The first step is to face joint one face, then edge joint one edge 90° to the jointed face. I also like to put a triangle on the edge so that I can keep the slats in order. Here is the milled blank ready to resaw.

My goal is to get four blanks—I only need three in the chair but I generally like to bend an extra one as a backup (sometimes even very small knots will put a kink in the slat while bending). This blank is roughly 2″ thick after jointing which will easily yield the four rough blanks, and probably five. If I am not concerned about getting the maximum number of slats from a blank I can simply set the band saw fence at 3/8″ or a little more. However, if I want to maximize the number of slats I can get from a blank I need to set up the fence for a more accurate cut. Brian can get 6 slats from a 9/4 board which makes one set of rocker slats or two sets of side chair slats. Especially if there is a distinctive grain pattern, it is nice to have all the slats from the same board in the order they were cut.

I will be cutting the slat mortises with a router which means the mortises will have a very consistent width of .250″ (1/4″), so I will mill the slat blanks to .270″ thick, enough extra width to fit the tenon precisely to the mortise. If you are hand chopping your mortises, depending on your skill level, the slat mortises may vary in width. In that case it is a good idea to mill the slat blanks a bit heavier, say .300″ thick, to allow for any variations in the width of the hand chopped mortises. Another issue to consider when thinking about what thickness to mill the slats to is the moisture content of the wood. For wood with a moisture content of between 12% and 20%, the above recommended thicknesses are fine. If the wood is much above 20% I will add .020" to .030" to the final milled thickness to compensate for the anticipated additional shrinkage when drying.

I generally like to resaw the blanks about .080″ thicker than the final slat width. If your band saw cuts very smoothly and accurately you can reduce that to about .060″ thicker. In this case I want my final slat blank to be .270″ thick, so I am aiming for a rough slat of about .350″ thick. Using a ruler I set up the fence as accurately as possible and then do a test cut. I use a small piece of scrap that is milled square on two sides (cut offs from prepping the rear legs work well for this). I draw a line on the scrap so I know the direction that the cut is made as shown on the left, then run the stock a short distance through the blade, pull it back out, and clip off the test cut to measure as shown on the right. If the width is off I manually readjust the fence, trim the test stock, and make another test cut. My second test cut measures almost exactly .350″, so I am ready to resaw.

I resaw each slat carefully and slowly. If the saw is cutting well there is no need to face joint between cuts. I stack the slats in the same order as they were cut as shown here.

Next I thickness plane the slats to final width. I take small cuts, moving the planer head down 1/4 turn after each pass (1/64″). I pay careful attention to the quality of the cut. If it looks like I am getting tear-out I rotate the blanks end-for-end before taking another cut. It usually takes about two or three passes on the first side to remove all the band saw marks. Then I flip the slats over end-for-end and take another two or three cuts. At this point I measure the thickness after each pass and stop when the slats reach their final thickness, which in this case is .270″.

Here are the five slats laid out in the order that they were cut. Sometimes the slats will have a distinctive grain pattern. In that case I may want to preserve the cut order so that the similarity in grain pattern can be seen from one slat to the next. In this case the maple slats have a very consistent grain pattern so that is not an issue. But they do have small areas of staining which I would like to end up in a similar area on each slat.

Because the grain pattern is so consistent I am at liberty to flip some slats over in order to move the area of staining. I also need to trim the length of the blanks from about 22″ to the final length of 20″. I can influence the location of the staining by trimming off the excess from one side or the other. Here are my choices for the four slats I will bend. The top slat has no staining at all, and the bottom three have staining in similar positions. To ensure that these slats are bent with this face down on the form I put a pencil mark on the left edge of each blank. This will help me orient the slat correctly when bending.

Here are four slats in a rack ready to be put in the steam box.

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #7: Steam Bending, Part 2

Using the steamers  |  Steam time  |  Moisture content for steam bent parts  |  Why use a bending strap  |  Bend the rear legs  |  Dry the rear legs

After the final, pre-bend milling of the rear legs they are now ready for the steam box. I like to start by adding boiling water, rather than cold water, to the steamers. This greatly accelerates the time it takes to get the steam box up to maximum temperature. I pre-boil the water in an electric kettle which holds about a half gallon, add it to one of the steamers, and repeat 5 more times until both steamers are full. In warm weather the steam box will get up to it’s maximum temperature of 200° in about 20 minutes. This is the maximum temperature that my thermometer registers under these conditions, but it may not be the actual temperature. Your thermometer may register a different maximum—just wait until the temperature stops rising before beginning to count the steaming time. I described my steam box set-up here. Of course you can use any source of heat and water container that will produce large volumes of steam.

Using the steamers

  • When full, my steamers will run for about an hour and a half before needing more water
  • Whenever adding water, I always boil it first, since adding cold water will lower the temperature considerably inside the steam box.
  • It’s very important that the steamers do not run out of water. If they do, they will shut themselves off and the only way to turn them back on is to cool them off first by filling them with cold water several times.
  • I always empty the steamers after I’m done. The one time I used water left over from a previous steaming session the day before, the oak slats I was steaming ended up getting stained pretty badly. I’m not sure exactly why this happened but I believe that the water left overnight reacted with the metal in the elements causing the same kind of staining you see from a rusty nail in an oak board.
  • If it is very cold be sure to thaw out the hoses before steaming. This past winter I steamed a pair of legs one day and the next morning set up the steamers again to steam some slats. I went inside the shop and a few minutes later I saw tons and tons of steam outside the window. It turns out that water inside one of the hoses froze overnight, preventing the steam from going through the hose into box. The steam needed to go somewhere, and fortunately the steamers have an emergency release valve, which was where all the steam was coming from.

Steam time

  • I begin counting the steam time when the temperature reaches maximum (on my thermometer it is 200°)
  • Steam maple, cherry and walnut legs for 2 hours
  • Steam oak legs for 3 hours
  • Steam hickory legs for 3-1/2 hours

Moisture content

  • The ideal moisture content range for bending is 12% to 20%. The maple legs I am bending today have a moisture content of about 18%.
  • If the moisture content is below 12% you can improve the chances of a successful bend by steaming the legs for an hour or so the night before. After steaming, keep the legs in the steam box overnight and keep the steam box closed. Then in the morning steam as usual, and begin counting the steam time when the temperature reaches maximum.
  • If the bending blanks have a moisture content much over 20%, I make the blanks about 1/16″ oversize in both width and height. The added dimension compensates for the additional shrinkage you can expect as the legs dry.

Steaming

  • In the post on final milling, the last thing I did was label the front face at the bottom of the leg with the word “UP”. Once the steam box reaches maximum temperature, I always put the legs into the steam box top of the legs first, with the front face (tapered side) facing up. Being consistent in this helps me keep the leg blank oriented correctly when I’m ready to put it into the bending form.
  • Close up the steam box and steam for the proper time for the species you are bending. In my case, I will steam the maple legs for 2 hours.

Bending

Heating wood to 200° or more with steam helps to loosen the lignin, a natural adhesive that holds wood fibers together, and allows the wood to bend and retain it’s shape after it has cooled and dried. In general, wood has a much greater capacity to compress rather than to expand. Wood fibers on the inside of the bend will compress. Wood fibers on the outside of the bend will want to expand and are more likely to break. A bending strap can prevent expansion of the outside fibers reducing the likelihood they will break. For the bending strap to be effective in preventing expansion it is critical that the leg be held very tightly between the two stops in the strap assembly.

Here is a video that shows the complete bending process. Each leg takes about 3 minutes start to finish. Or view directly on YouTube.

Drying

Initially the leg is overbent. The purpose of the overbend is to deform the fibers which reduces the likelihood of spring back as the fibers relax to their final shape while drying. I leave the leg in the overbent position for a few hours as shown here.

After several hours I move the pin to the upper position in the gusset and allow the leg to rise to it’s final shape as it dries.

Another option is to move the leg to a drying form. The drying form is identical to the bending form except that it has no bending strap. The only other difference is the position of the pins in the lower gusset—they are 1″ lower compared to the bending form to compensate for the lack of the handle assembly. There are a couple of reasons to use a drying form. The first is that I only have two bending forms and I might need them to bend more legs. Secondly, the drying form exposes more wood to the surrounding air, which can aid in drying.

Since I do a lot of bending I built a dedicated drying closet into a corner of my shop. The dimensions were determined by the space I had available—approximately 27″ wide by 18″ deep. If I had more space I would probably make it a little larger. It can hold a maximum of 3 pairs of legs, but usually I dry a pair or two pairs of legs along with their slats. I insulated the two walls with 1″ Styrofoam. The wall on the left has a 1″ gap at the bottom and the top to facilitate air movement (I’m not sure if this actually works, but it seems like a good idea). The heat source is a small oil filled radiator. I generally try to maintain a temperature of around 100° or so. Under these conditions most legs will be dry and ready to work in about a week. Soft maple dries very quickly and will probably be ready in a few days. On the other hand I have had some oak legs take two weeks or more to dry. As you can see here I have transferred the legs to a drying forms.

It is not necessary to have a dedicated drying closet like this. Find a warm spot, such as a furnace room or behind a wood stove in winter, and dry the legs there. If you don’t have a warm spot the legs will simply dry more slowly. During the first class I took with Brian, we even dried slats in the back of someone’s hatchback on a sunny day.

Next up in the blog I will mill slat blanks prior to steam bending.

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #6: Steam Bending, Part 1

Steam generation  |  Steam box  |  Rear leg bending form  |  Sources for steam bending supplies

Steam bending is a wonderful, almost magical, way to make curved parts. In a matter of hours I can transform what looks like a completely unbendable rough board more than 2″ thick into a beautifully curved chair leg ready for final shaping. The process uses material efficiently, especially compared to cutting out the same shape from a flat board. And, if I have been careful about orienting the long grain parallel to the sides of the blank, the grain will wrap around the bend making for a very strong leg with little or no run out. Although there are occasional bending failures (some wood just won’t bend even if it is a species that normally bends well), a careful and methodical process can yield very predictable results.

As described in previous posts, here,  here, and here, steam bending really begins with careful wood selection and preparation. Once that is complete I am ready to bend. Here is a photo of my dedicated steam bending set up on the front porch of my shop. I like having it outside so I don’t have to deal with the effects of lots of steam inside the shop. It is also under cover so I can comfortably bend in all weather. The box is not insulated, but even in cold weather, once it reaches maximum temperature it stays there for the entire steam time.

Generating steam

I use two steamers made by Earlex. Rockler also sells a steamer that I believe is identical, except that it comes with some additional hardware for building a steam box. As far as I know these are essentially wallpaper steamers sold as steam generators for wood bending, hence the very long hose. They do come with fittings that allow for easy connections between the hose, steamer and box. Of course anything that will generate a large volume of steam will work, such as a large pot heated by propane. I prefer these electric steamers since I can simply plug them in and I never run out of fuel.

I’m not really clear about the science behind it, but as I understand it, large volumes of steam moving through the box do a really good job of transmitting heat to the part. It is the heat, not the moisture, that makes the wood fibers pliable enough to bend. For a box this size I find that two steamers work very well, producing a very large volume of steam. If you want to use one steamer, I would consider reducing the dimensions of the box. For instance this box can hold 4 rear legs, so you could reduce the height of the box by half and still be able to hold 2 rear legs. I can’t say for sure this will work since I have never tried it, but that’s where I would start.

Each steamer uses 1500 watts of electricity and requires it’s own 15 amp circuit. The outlet I installed, lower right, is actually 2 separate 15 amp circuits, one for each steamer.

Steam Box

  • 48″ long by 6″ wide x 6″ tall, interior dimensions, made from exterior plywood. This box can hold 4 rear legs or 6 slats.
  • The long sides are caulked and air tight. The two doors are not air tight and allow steam to escape. This is extremely important since an air tight box would explode with the pressure created by the steam. Additionally the movement of steam through the box seems to help transmit more heat to the parts.
  • The left side of the box is slightly elevated to encourage drainage through a small hole on the bottom, right side of the box.
  • I put a small thermometer towards the top on the left side of the box. When the temperature reaches 200° I begin counting the steam time. I’m not sure if 200° is the actual temperature inside the box, but it is the maximum this thermometer registers under these conditions. Other thermometers may register a different maximum temperature, so wait until the temperature stops rising before beginning to count the steam time.
  • For longer parts (the rocker legs are almost 50″ long) I open the door on the right and extend the length of the main steam box by sliding a smaller box in the open end. You can see this box sitting on top of the steam box towards the right. If I were building the steam box over again I would simply make it a little longer.

Bending Form

The other essential element in steam bending is, of course, the bending form, pictured below. This form is designed as both a bending form and a drying form. The main bend in the center of the form actually applies an overbend to the leg, which is held in the overbent position for several hours. After that the leg is allowed to rise to it’s final position to dry. The purpose of overbending is to minimize spring back as the leg dries to it’s final shape. A long metal pipe can be slipped over the handle on the right should I need additional leverage when bending. The distance between the top swivel stop on the left and the bottom stop in the handle on the right matches the length of the leg blank.

Pictured below is the end of the form that captures the top of the leg. This stop swivels to make it easier to insert the straight blank into the form. Below the top stop is a french cleat for hanging the form. Attached to the swivel stop by 2 bolts is the 2″ wide bending strap. Above the strap is a thin piece of oak which protects the leg when clamping it to the form. And, below the bending strap is a 2″ wide piece of thin stainless steel which keeps the leg from contacting the steel bending strap, thus minimizing or eliminating any staining. The cutout on the bottom of the form is for clamping.

And here is the end of the form that captures the bottom of the leg. The gusset has two locations for pins. Initially a pin is put in the lower location to hold the leg in an overbent position. After several hours the pin is moved to the upper location allowing the leg to gradually rise to it’s final shape while drying. The bending strap is bolted between the two parts of the handle assembly. If you look closely you’ll see a small notch cut out of the left side of the lower handle. The stainless steel slips into this notch but is not bolted to it. This keeps all of the bending pressure on the bending strap itself which is designed to handle it, and doesn’t stretch out the stainless steel which is allowed to move freely in the notch.

An alternative to the wooden handle assembly pictured above is this strap clamp, shown below. The benefit of the strap clamp is that it opens up to easily fit over the blank then tightens to a very sung fit between it and the swivel stop at the top of the leg. The wood fibers at the top of the bend will want to expand while being bent. A very snug fit between stops allows the bending strap to put lots of downward pressure on the blank, keeping the fibers at the top of the bend from expanding and breaking. The strap clamp is capable of applying more pressure on the bending strap compared to the wooden handle assembly so if you are having problems with the blank breaking at the top of the bend using a strap clamp may help. The only downside is that it is a good deal more expensive than the wooden handles. In the side chair class that I teach, and in the forms that I help my students build, I always use the wooden handle assembly since it is less expensive and generally works very well.

Sources

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #5: Preparing the Rear Legs for Bending

Understanding ideal grain orientation for the rear leg blanks  |  Transforming a rough milled rear leg blank to a final blank ready for steam bending

Updated April 5, 2020

Once I have all the rough blanks for the chair milled I am ready to prepare the rear legs for steam bending. As with most things in the process of building this chair there is more to it than simply cutting the parts to specific dimensions. You may recall when I milled the rough blanks for the rear legs I was looking for pairs of legs with straight long grain and matching rift sawn end grain. In taking the legs from a rough blank with those characteristics to a finished pair of legs ready-to-bend, I am primarily concerned with finding the optimal grain orientation (both end grain and long grain) for the pair. A secondary concern is to mill out or minimize defects, if any, in the blank.

Orienting the end grain of the legs so that it is rift sawn is done to make the best possible leg to rung joint. In my second post on grain orientation I explained that when you add the angle of the rift sawn end grain to the angle that the legs are rotated by the slats during assembly the result is end grain that is roughly 45° relative to the long grain of the rungs, which makes for a good leg to rung joint. Pictured below, on the left, are a pair of legs from the rift sawn board. The end grain on these blanks have an angle greater than 45°, so the simple solution to make them rift sawn is to rotate each leg 90°. Pictured on the right is the result. Ideally the rift sawn end grain in each leg will be a mirror image of the other, as it is here. 

Orienting the long grain at the top front face of each leg is done for aesthetic purposes. The object is to have the long grain mirror or complement the physical angle of the legs themselves. The rear legs are further apart at the top and closer together where they meet the seat, so, when viewed from the front, the legs angle toward the center of the chair. I want the long grain in each leg to also angle towards the center of the chair. Grain that is parallel to the length of the leg is also a good option. Each blank has four potential top front faces. To find the combination that works best I move the blanks to various positions relative to each other and choose the combination works the best. In the photo below, left, I have highlighted the long grain with pencil to make it easier to see. The top two feet of these blanks has long grain that angles slighty toward the center which is what I am after. The photo on the right shows my final choice for orientating these two blanks—rift sawn end grain that is a mirror image on both blanks and long grain on the top front face that angles slightly towards the center.

Other considerations, beyond grain orientation, include identifying any defects, which can include small knots, grain runout, and in this case, staining. Anticipating the upcoming steps in transforming these blanks to finished legs I can use the milling and shaping process to minimize or eliminate defects. For instance, in the blank on the left, there is staining on the top, front face that I don’t want to appear in the final leg. The staining penetrates the blank about half an inch. There are several things I can do about this. First, the blank is roughly 2-1/4″ square and the final thickness, front-to-back is 1-5/8″, so I know I can mill almost half an inch of material from front face. If that is not enough, I also know that the top front face has a taper cut into it, removing even more material. I can also use the fact that I will be trimming the blank to length (from about 48″ to 45-3/16″) to affect the location of a defect by trimming mostly from the top or mostly from the bottom. Additionally, after bending, I will trim about 3″ from the top of the leg and about 1" from the bottom so I know that any defect in these sections will be removed.

Once I have made all the choices regarding the orientation of each blank I am ready to begin milling. The blanks are roughly 2-1/4″ square in cross section. The final milled dimensions are 1-5/8″ front-to-back and 1-7/8″ side-to-side. The side-to-side dimension is 1/4″ wider than the final dimension of the leg—bending often introduces some twist into the blank and this extra width will allow me, after the blank is bent and dried, to joint one edge flat and thickness to 1-5/8″. To make it easier to keep track of which dimension is which I label each blank with an arrow and a “5” (for the 1-5/8″ dimension) and an arrow and a “7” (for the 1-7/8″ dimension) as shown below on the left. I also point the arrow toward the face that I want to joint. I begin by face jointing the sides identified by the arrow and “5”. Next I edge joint the sides identified by the arrow and “7”. These become my two reference edges. At this point there are couple of different ways to mill to final size, depending on the equipment you have available. One way is to rough mill the blanks to about 1/8″ oversize in both dimensions on the bandsaw (keeping the reference edges against the fence and the table when cutting) and then mill to final dimensions on the thickness planer. A second way is to mill to final dimensions on the table saw, again being sure to always have the reference edges against the fence and the table. Pictured on the right are the blanks milled to final dimension. By taking most of the material from the front face I completely eliminated the staining on the left blank. There was also some light staining on the sides of each blank so I was careful to mill in a way that removed all of it.

The next step is to trim the blanks to length (45-3/16″). This is my final opportunity to affect the location of any defects. In this case, having no defects to consider, I simply squared up the tops and trimmed to length by cutting from the bottom.

Finally I will cut a taper into the front face at the top of each blank. I begin by laying out the cut. Even though I will make this cut on a taper jig, I always lay it out completely to ensure that I put the blank in the jig correctly. The first mark is 22″ from the top on the front face (upper right in the photo below). The second mark is 1″ from the back face on both sides of the blank. Next I connect the marks as pictured. The result will be a 5/8″ x 22″ taper milled off the top, front face of the blank. I always save the cutoffs—the long, thin wedges often come in handy.

Here are a couple of shots of my dedicated table saw taper jig. It only cuts 5/8″ x 22″ tapers which are used in both the side chair rear legs as well as the rocker rear legs. There is a long base that is 7-1/2″ wide. Attached to the base is a fence 22″ long and 1-5/8″ from the left side of the base. Toward the bottom of this fence is a screw that projects 5/8″ from the fence and a stop to capture the blank. And there are two hold-downs to secure the blank tightly in place. Pictured at right is the blank in the jig ready to be cut with the layout lines showing the off cut. I very carefully make the cut using a push stick along with outfeed support beyond the table to support the leg as the cut is made. There are many other ways to make this taper cut depending on the equipment you have available and your comfort with particular processes. The easiest is to rough cut the taper using a bandsaw, then clean it up smooth and flat with a handplane. There are also scary and non-scary ways to make this cut on jointer. And, finally the entire cut can be made with a drawknife and spokeshave if you would prefer using hand tools. I chose the table saw taper jig because it is fast, accurate, safe, and I have proper equipment.

The final blanks, ready for the steam box, are pictured below. On the left I’ve turned the blanks on their side to reveal the profile of the taper cut. On the right I’ve highlighted in pencil the rift sawn end grain at the bottom, and the long grain on the front face of the taper cut. The taper cut altered the angle of the long grain slightly, giving it a more pronounced angle towards the center, which I really like. I also labeled the bottom front face with the word “UP”. I put the legs in the steam box with the front face up and I also put the front, tapered face up in the bending form. Even with the taper it is difficult to distinguish front from back (especially when I am moving quickly to bend the leg) so this simple label helps me get the orientation of the leg correctly in the bending form. All-in-all, two near-perfect rear leg blanks. Although this explanation is quite lengthy, the actual process of milling ready-for-steaming legs blanks from rough blanks goes very quickly.

In my next post I’ll describe my steam box setup and bending form. Stay tuned.

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #4: Milling Blank Parts, Part 2

Choosing a quarter sawn board for slats  |  Layout and mill a slat blank  |  Layout and mill the front leg and rung blanks

Updated April 5, 2020

After milling the blanks for the rear legs I turn my attention to the slat blanks. For the best joint I use wood with quarter sawn end grain. When assembled, the radial plane in the slat tenon will run parallel to the long grain in the leg which makes the mating parts of the joint as compatible as possible. The quarter sawn board pictured at the beginning of the last post has more than 5″ of clear, quarter sawn end grain on both sides of the board. I have cross cut the piece pictured below to about 22″ in length from that longer board. I generally look for a blank that is clear and free from defects. This board has no defects and straight long grain so it’s perfect for slats. It’s possible to use wood with very small defects or very small knots, but occasionally while bending the slat will kink at the point of even a small knot.

To layout, I draw a reference line parallel to the bark edge and then a second line about 5″ away and parallel to it. I freehand cut both layout lines on the bandsaw as shown with the blank on the right. With careful milling this blank will yield up to 6 slats, enough for two side chairs or one rocker. Because I am building one chair I won’t cut out the second slat blank at this time. The rift sawn wood remaining in the center is perfect for front legs and rungs.

Once I have cut out blanks for the parts that require specific end grain orientation—rift sawn end grain for rear legs and quarter sawn end grain for slats—I am ready to mill blanks for the front legs and rungs from the wood that remains. Pictured below is the 2ʹ long butt end section of the rift sawn board that I used for the rear legs. This piece has quite a bit of flair toward the butt end so I am very careful to layout the parts as parallel to the long grain and the bark edge as I can. I am aiming for straight long grain with as little run-out as possible. Front legs can have small defects. I am not concerned with the end grain orientation because these parts are straight and cylindrical so they can be rotated to the correct grain orientation at the time of rung mortising (front legs) or assembly (rungs). This piece will yield 4 front legs and 4 pairs of rungs.

Here is the same board cut into parts. I actually got an extra pair of rungs so the total from this piece is 4 front legs and 10 rungs. The only reason the wedge shaped section in the center is waste is because of the staining. Otherwise I could have gotten another front leg or some more rungs.

And finally a photo of all the parts for this chair: 2 rear legs with rift sawn end grain, 2 front legs, a slat blank with quarter sawn end grain, 7 lower rungs in soft maple (including 1 extra) and 5 seat rungs in hickory (including 1 extra). In the finished chair the seat rungs must hold up to the enormous strain of the seating material wrapped around them and the weight of someone sitting in the chair. If the primary wood is relatively soft I used a harder wood such as hickory, white oak, ash, or hard maple for the seat rungs. Species that are not strong enough to be used as seat rungs include soft maple, cherry and walnut.

In the next post I will demonstrate how to mill a rear leg blank for steam bending.

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #3: Milling Blank Parts, Part 1

Choosing a rift sawn board for the rear legs  |  Layout the rear leg blanks  |  Mill the rear leg blanks

Updated April 5, 2020

Now that I have milled or located good chair wood it’s time to start building the chair. The first step is to mill the blank parts out of the sawn lumber. This is more than simply cutting parts to size. Each board is evaluated to determine it’s suitability for various parts. And each part is laid out for optimal end grain orientation. I use rift sawn boards for rear legs and quarter sawn boards for slats.

Here are two heavy 9/4 (about 2-3/8″ thick) soft maple boards. The top board has nice rift sawn grain and is about 15″ wide at it’s narrowest point, enough to get 3 pairs of rear legs. The bottom board, about 18″ wide at it’s narrowest point, has wide areas of quarter sawn end grain on both sides that will be perfect for slats. If I only had the bottom board, I could also get a pair of rear legs from it—the slat blanks need about a 5″ width of quarter sawn end grain, and to the inside of this there is enough rift sawn end grain for a pair of rear legs. Since I have both boards I’ll simply take the rear legs out of the top, rift sawn board and the slats out of the bottom, quarter sawn board. Front legs and rungs have less demanding requirements and will be cut after the rear legs and slats from the wood that remains.

First, I check the moisture content of the boards. For parts that will be bent (rear legs and slats) the ideal range of moisture content is from 12% to 20%. It’s possible to bend wood with a higher moisture content, but you must compensate for additional shrinkage as the wood dries by increasing the thickness of the blank. And, if the moisture content is too low there are ways to increase it before steaming. The moisture content of these two boards is about 18% which is perfect for steam bending. Front legs and rungs will not be bent so a lower moisture content is better. For those parts I sticker and stack them in the shop and let them acclimate to the interior environment. After that I may also put them in a small kiln to get them down to final moisture content which in my shop is about 8%.

For rear legs the goal is a bending blank with these specifications: 4ʹ long, rift sawn end grain, very straight long grain, and no defects. I start by laying out the cuts for the rear legs on the rift sawn board. This board is remarkably free of knots and other defects and has very straight long grain running parallel to the bark edge. It does have a large dark stain running vertically down the center that I will not be able to use. There is also some light gray staining across the width of the board in the center—the shed where I stacked this lumber leaks and the board got wet causing the stain. Fortunately the light staining is only on the surface so I’ll be able to remove it in the milling process. This board is roughly 6ʹ long. As you can see it flairs dramatically toward the butt end so I’ll take the rear leg blanks out of the top end which is straighter. First I layout a horizontal line 4ʹ from the top—this is where I will cross cut the board in two. The 2ʹ long section at the bottom will be used for front legs and rungs. The straightest grain runs parallel to the bark edge so I draw a reference line as close to, and parallel to the bark edge. For species with sap wood that differs in color from the heartwood, such as walnut or cherry, I draw the reference line parallel to the bark edge at the point where the sapwood ends and the heartwood begins. Next I layout out lines parallel to and about 2-1/4″ away from the reference line for each blank. On this board I will get 3 legs on either side of center as shown here. I was very lucky to avoid the stain in the center, but even if this board had no stain or defect in the center I would still lay out the blanks the same way.

Here is a shot of the same board after cross cutting to 4ʹ in length. The safest way for me cross cut a board of this size is with a jig saw. You can clearly see the rift sawn end grain in each blank. Rift sawn end grain has growth rings that are 45° or less. If the end grain in the blank is greater than 45°, as is the case with the two outermost pieces, I will simply rotate the blanks 90° before final milling so that the growth rings are less than 45°. The two outermost blanks make up a pair since the end grain in each will mirror each other in the final chair. The same goes for each succeeding pair of blanks. I have labeled the pairs in the bottom photo.

I do the balance of the milling on the bandsaw. First I freehand cut along both layout lines in the center of the board, mainly so I can work with smaller, more manageable pieces. Next I edge joint the freehand cuts, set up the bandsaw fence for 2-1/4″, and rip cut the remaining blanks. The fully milled board is below. Because I cut parallel to the bark edge, the long grain is as straight as possible. What’s left is the bark edge, which ends up in my woodstove, and the wedge shaped piece in the center. Often the wedge in center can be used for front legs and rungs, but in this case the stain limits what I can do with this piece. There may some clear wood on the reverse side for a rung or two. 

In the next post I’ll go over milling blanks for slats, front legs and rungs. Slats are best cut from quarter sawn wood. After milling the rear legs and slats there is usually enough wood left over for front legs and rungs which are easier to find because those parts are relatively short and don’t require a specific grain orientation out of the board.

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #2: Logs and Lumber

Evaluate a log’s suitability for chair wood   |  Mill a log for the best grain orientation for each chair part  |  Mill for the most efficient use of each board

Updated April 5, 2020

Building a Boggs side chair usually begins with selecting and milling a log. This approach puts you in control of the process all the way back to the log. If you do not have access to logs or a sawyer I will talk about alternatives at the end of this post. There are a variety of wood species that work well for this chair—maple (soft or hard), walnut, cherry, white oak, red oak, ash, and hickory. Since chair wood requires very straight grain I look for logs with these characteristics:

  • very straight with no bends, as close to a cylinder as possible, although all logs will taper from one end to the other

  • the furrows in the bark should run straight up the log. If the furrows spiral up the log it is often an indication that the grain within is twisted

  • no indication on the surface of any large branches

  • 15″ to 18″ minimum diameter, larger if possible

Here is a nice walnut log ready to be sawed.

I have been very fortunate to develop a relationship with a local sawyer, Rick Herbine of Herbine Hardwoods, in Leesburg, Virginia. He knows the species and characteristics I am looking for and lets me know when he has a log that matches them. Then at his mill he saws the log while I’m there so that I get exactly the cuts I’m looking for.

It is critical to have straight long grain so the first step, after selecting a log, is setting it on the mill and leveling the centers at each end relative to the path of the blade. This is very important as it ensures that, at the center of the log, the board is cut exactly parallel to the long grain. Here is an oak log that has been sawed in half. This log has a pronounced taper from the larger butt end on the left to the smaller diameter of the end on the right. If you look under the right end you’ll see a block raising it up so it’s center is at the same height above the bed as the end on the left. The surface of this cut is now parallel with the long grain of the log.

In addition to straight long grain, the other goal when cutting the log is to get boards with the correct end grain orientation for specific chair parts such as slats and rear legs. Slats use quarter sawn wood (growth rings roughly 90° relative to the width of the board), and rear legs use wood that is rift sawn (growth rings that are 45° or less relative to the width of the board). The grain orientation does not matter for front legs and rungs—those parts are round in cross section and can be rotated to the proper grain orientation at the time of rung mortising or assembly.

Here’s how I mill a log into boards.

If you have any doubt about your ability to cut accurately and without waste you should consider milling the boards at the thicker dimensions shown above.

After milling slats from quarter sawn boards and rear legs from rift sawn boards there is usually wood left over that can be used for front legs and rungs.

I generally leave the bark edge on the boards—the best and straightest wood runs parallel to the bark edge which becomes a reference when milling leg, slat and rung blanks.

An 8/4 or 10/4 board that is 18″ wide and 8ʹ long is very heavy, especially when it is green. Recently, on thicker boards I’ve been having the sawyer cut the boards lengthwise down the center along the pith and cross cut them to length. This reduces a large board to several smaller pieces which are much easier to handle. For an 8ʹ to 9ʹ long board I cross cut in half to 4ʹ to 4-1/2ʹ. For a 6ʹ long board I cross cut at 4ʹ and 2ʹ. And for a 10ʹ long board I usually cross cut two boards at 4ʹ long and one at 2ʹ long. You can get any chair part out of a 4ʹ long board. And you can get rungs, front legs, and slats from a 2ʹ long board.

Once the boards are milled you’ll need to sticker them and let them dry. For wood that will be steam bent the ideal moisture content range is from 12% to 20%. You can accelerate the drying for rear leg blanks by cutting rough blanks, roughly 2″ x 2″ x 48″ and letting those dry. The exposed wood on the sides will aid in drying more quickly. If you must use wood that has a moisture content higher than 20% be sure to add about 1/16″ in dimension to the width and height of the bending blank to account for additional shrinkage.

Here is one of the boards milled from the walnut log—beautiful, straight, long grain that will be perfect for chair parts.

Milling your own boards from logs that you select is the best way to get great chair wood. But what is the alternative if you can’t find a sawyer to work with. For rear legs and slats it is best to find a source of air dried lumber. It is possible to bend kiln dried wood and I will be experimenting with that in the near future, but air dried wood, if you can get it, is always the better option. When using kiln dried wood be sure to look for boards with straight long grain and the correct end grain orientation—quarter sawn for slats and rift sawn for rear legs. Also, with any boards with a sawn edge, don’t assume that the long grain runs parallel to the sawn edge. Always look at the long grain of the board and if necessary saw a new reference edge parallel to the long grain.

Here are two sources of chair wood. They will both will ship wood if you are not close to them.

Herbine Hardwoods, Leesburg, Virginia. Rick Herbine is wonderful to work with and over the years I have bought many logs, all milled to my specs. Take a look at his web site or give him a call at 703-771-3067.

Robert Carran, Asheville, North Carolina. Robert used to work for Brian and has an intimate understanding of milling logs for the best chair wood. Give him a call at 828-319-7756.

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More
Boggs Side Chair Build Jeff Lefkowitz Boggs Side Chair Build Jeff Lefkowitz

Boggs Side Chair Build #1: Introduction

Welcome to a series of posts that will describe how to build a Boggs 3-slat post and rung side chair.

A student built 3-slat post & rung side chair in white oak

A student built 3-slat post & rung side chair in white oak

Updated April 5, 2020

Welcome to this series of posts that will describe how to build a Boggs 3-slat post and rung side chair. Brian designed this chair to fit a human form as comfortably as possible and, if you build one, it will surely be one of the most comfortable wooden chairs you ever sit in. Although the design has its roots in traditional Appalachian ladderback chairs, its graceful curves allow it to look at home in contemporary as well as traditional settings.

Over the years Brian has refined the process of building ladderback chairs. The processes I will describe in this build series are a combination of Brian’s methods and ones I’ve refined and developed over many years of teaching students of all skill levels how to build this chair. Together the methods to build this chair and the principles behind them form an excellent introduction to the craft of ladderback chairmaking.

I will start at the beginning with log and lumber selection and move through the process in a stepwise fashion. Along the way I will explain in detail every aspect of building this chair including steam bending, shaping parts with draw knife and spokeshave, turning, drilling angled mortises into curved parts, understanding grain orientation and wood movement, assembly with hide glue, seat weaving, finishing, and more. I will also venture into related topics such as tool sharpening and maybe even making some custom chairmaking tools.

Students working in my shop in Strasburg, Virginia

Students working in my shop in Strasburg, Virginia

Over the past eight years I have been teaching students how to build this chair in seven day classes in my shop in Strasburg, Virginia. There are some concepts, such as drilling angled rung mortises, where the process is simple to execute but the underlying principle is difficult to explain. For me, the classes have been an ongoing opportunity to refine and perfect how to communicate in ways my students (and you) can understand. In working with students I have found it is very helpful to break down each process into small, discrete, doable steps. The student focuses on doing that small step well before moving onto the next, each step building on the last. And there have been times where I’ve expanded or modified the steps after watching a student struggle. These refinements in process become part of the way I teach. For this series I will describe processes in much the same way as I do in class—in a step-by-step methodical fashion, explaining how-to, pointing out pitfalls, showing you what to look for and how to evaluate what you’ve done.

My hope is that this series will become a comprehensive reference on how to build a ladderback chair using the methods that Brian has developed and I have refined and added to. I encourage you to comment and ask questions as we go. Building a chair like this is a very satisfying experience—and the payoff is lots of new skills and a comfortable, hand made chair to sit in once you’re done!

Jeff Lefkowitz

 

Side Chair Build Series Links:

 

Read More